Analysis and Discussion on the process of powdered lithium ion battery production

Release:xxshldy browse:3667

The production process of lithium cobalt oxide is basically not powdered. The factors that affect the production process are:

1, improper formulation, such as too few adhesives, less capacity, resulting in uneven mixing.

2, the temperature of adhesive baking is too high, so the structure of the adhesive is destroyed.

3, slurry mixing time is not enough, not fully stirred.

4. The temperature of the coating is too low and the pole is not dried.

5, the coating quantity is not uniform, the thickness difference is too big.

6. The pole piece does not bake before rolling, and absorbs water in the air.

7. When the roller is pressed, the pressure is too high.

8. When the roller is pressed, the way of sending the pole pieces is not correct, resulting in uneven stress of the pole piece.

9. With oil positive pole, water negative pole, no powder?

Three. Bad battery projects and causes:

1. low capacity

Cause:

The amount of A. is less than that of the B. pole; the difference between the two sides of the pole piece is quite different; the C. pole piece is broken.

The electrolyte of D. is less, the conductivity of E. electrolyte is low, and the positive electrode of F. is not matched with the negative electrode.

The porosity of the g. membrane is small, the H. adhesive is aging and the attached material falls off, and the I. core is super thick (not dried or the electrolyte is not permeable), and the J. is not full of electricity, and the K. positive and negative material is smaller than the capacity.

2. high resistance

Cause:

A. negative electrode and polar ear arc welding; B. positive electrode and pole ear welding; C. positive pole and cap virtual welding; D. negative electrode and shell welding; e. rivet and pressure plate contact internal resistance; F. positive pole without conductive agent; g. electrolyte without lithium salt; h. battery has short circuit; I. diaphragm paper porosity is small.

3. low voltage

Cause:

A. side reaction (electrolyte decomposition; positive electrode with impurities; water); B. not good (SEI film is not safe); C. customer's circuit board leakage (refers to the client after processing back of the electric core); D. customer is not required to spot welding (customer processed core);

E. burr; F. micro short circuit; g. negative electrode producing dendrite.

4. the causes of ultra thick over thickness are the following:

A. seam gas leakage; B. electrolyte decomposition; C. not dried water; D. cap sealing poor; e. shell too thick; F. shell too thick; g. coils too thick (too much material; no compacted pole; too thick diaphragm).

The 5. causes have the following points

The A. is not good (SEI film is incomplete and dense); the baking temperature of B. is too high and the binder aging and decharging; C. negative electrode has low specific capacity; D. positive electrode is more material and less negative material; e. cap is leaking, welding seam gas leakage; F. electrolyte decomposition, conductivity decrease.

6. explosion

Failure of A. capacity cabinet (causing overcharge); poor closure effect of B. diaphragm; internal short circuit of C..

7. short circuit

A. material dust; B. shell fashion broken; C. scrape (small diaphragm paper too small or not padded); D. winding is uneven; e. is not wrapped; F. diaphragm has holes; g. burr.

8. circuit breaker

A) the pole ears are not welded well with the rivets, or the area of the effective solder joints is small.

B) the joint piece is broken (the joint is too short or too far down when the spot piece is welded.

Four, the safety characteristics of lithium ion batteries

Li ion battery has been widely used in people's daily life, so its safety performance should definitely be the first assessment index of lithium ion battery. For the evaluation index of the safety performance of lithium ion batteries, a very strict standard has been stipulated in the world. A qualified lithium ion battery should be satisfied with the safety performance.

1) short circuit: no fire, no explosion;

2) overcharge: no fire, no explosion;

3) hot box test: no fire, no explosion (150 10min constant temperature)

4) Needling: non explosion (using a 3mm nail to penetrate the battery);

5) flat plate impact: do not fire, do not explode; (10kg weight from 1 meters high to hit battery)

6) incineration: non explosion (gas flame burning test battery)

In order to ensure the safe and reliable use of lithium-ion batteries, experts have carried out very strict and detailed battery safety design to achieve battery safety assessment indicators.

1, diaphragm 135 degrees automatic shutdown protection: the use of advanced international Celgard2300PE-PP-PE three layer composite membrane.

2. Under the condition of the battery heating up to 120 C, the PE membrane holes on both sides of the composite membrane are closed, the internal resistance of the battery is increased, and the inside of the battery has a large area of circuit breakage, and the battery is no longer heating up.

3, the battery cover composite structure: the battery cover adopts the notch explosion-proof structure, when the battery temperature rises, the pressure reaches a certain degree, the crack breaks and deflate.

4, various kinds of environmental abuse test: carry out various misuse tests, such as external short circuit, overcharge, needle, plate impact, incineration, and so on, to investigate the safety performance of the battery. At the same time, the temperature impact test and vibration, drop and impact tests of the battery were carried out to investigate the performance of the battery in actual use.

HOME| ABOUT US| PRODUCT| TESTING INSTRUMENT| NEWS| APPLICATION| CERTIFICATION| FACTORY ENVIRONMENT| CANTACT

Copyright © Xinxiang Hongli Supply Source Technology Co., Ltd. All Rights Reserved. [MANAGE]

Address:The west section of Taihang North Road, Xinxiang Economic Development Zone, Xinxiang County Tel:0373-5632158

Shen Manager:13803735632 E-mail:hldy5632158@163.com

主站蜘蛛池模板: 亚洲成av人片在线观看无码| 精品一区二区三区视频在线观看| 毛片网站免费在线观看| 亚洲黄色小视频| 365深夜福利在线观看| 久99久精品免费视频热77| 大学生特黄特色大片免费播放| 免费a站| 欧美激情αv一区二区三区| 日本亚洲成高清一区二区三区| aaaaaaaaa在线观看| 网站在线播放| 亚洲日韩第一页| 日韩资源在线| 欧美大片天天免费看视频| 日本a一级| 牝性 ペルソナ| 在线观看高清免费| 青青草国产精品欧美成人| 91精品在线免费观看| 痴汉电车h漫画乃梨子漫画| 99久草| 青青草视频免费在线| 国产中文欧美| 欧美片免费观看网址| 羽田桃子| 四虎4hu影库永久地址| 欧美日韩亚洲视频| 欧美成人精品免费播放| 1区1区3区4区产品乱码区| 特雷弗亨德森所有作品| 91精品在线免费观看| 国产精品 主播精选 网红| www视频免费在线观看| 痴汉电车侵犯女教师| 免费1级片| 一区二区三区在线播放| 欧美色欧美亚洲另类二区| 心情好的日子国语版在线观看| 欧美国产综合视频在线观看| 黄色毛片免费网站|